跳到主要内容

Bambu Lab and Creality K1 high-speed profiles

An advertised maximum, such as 500–600 mm/s, is not the setting for a sign face. Limit the visible surface with outer-wall speed and volumetric flow. Push infill and inner walls toward the machine limit.

The numbers are starting values for a 0.4 mm nozzle, dried general-purpose PLA or PETG, and a machine that already has input shaping and Pressure Advance. If you exceed the stock hotend's flow limit, a higher speed number still leaves sparse walls.

Placement rules for split parts are in Sign splits.

Calculate the flow limit first​

Volumetric flow (mm³/s) ≈ line width (mm) × layer height (mm) × speed (mm/s)

For a 0.4 mm nozzle, 0.45 mm line width, and 0.20 mm layer height:

Outer-wall speedRequired flowDecision
100 mm/s9 mm³/sComfortable on stock PLA
150 mm/s13.5 mm³/sNear the PLA ceiling on some machines
250 mm/s22.5 mm³/sDo not use this on an outer wall with a stock 0.4 mm hotend
400 mm/s36 mm³/sHigh-flow hotend, infill only

Measure that filament's maximum volumetric flow before you raise outer-wall speed. Cap the outer wall at 80% of the measured value.

PLA starting profile​

Layer height 0.20 mm, outer line width 0.42–0.45 mm, 3 walls, 15% infill.

ItemBambu Lab X1 / P1Creality K1 / K1CK1 Max
Nozzle215–220°C215–220°C215–220°C
Bed55°C55–60°C55–60°C
Outer wall100–140 mm/s80–120 mm/s100–140 mm/s
Inner wall200–300 mm/s150–220 mm/s180–260 mm/s
Infill270–350 mm/s180–250 mm/s220–300 mm/s
Outer-wall acceleration5,000–8,000 mm/s²3,000–5,000 mm/s²4,000–6,000 mm/s²
Infill acceleration10,000–20,000 mm/s²8,000–12,000 mm/s²8,000–15,000 mm/s²
Cooling60–100%70–100%70–100%
Flow cap (stock)18–22 mm³/s15–18 mm³/s16–20 mm³/s
RetractionAdjust the machine default by no more than ±0.2 mm0.8–1.2 mm, around 40 mm/sStart from the same family as K1

Bambu defaults are already aggressive. For sign work, lower only the outer wall and top surface to this table and leave the rest of the machine profile. That is more repeatable. On the K1 family, do not take infill past 250 mm/s until input shaper and the flow test are finished.

PETG starting profile​

For indoor-outdoor brackets, clips, and damp installation sites. Keep the outer wall slower than PLA.

ItemBambu Lab X1 / P1Creality K1 / K1CK1 Max
Nozzle245–255°C240–250°C240–250°C
Bed70°C70–80°C70–80°C
Outer wall60–100 mm/s50–80 mm/s60–90 mm/s
Inner wall120–180 mm/s100–150 mm/s120–160 mm/s
Infill160–220 mm/s140–180 mm/s150–200 mm/s
Cooling30–60%40–70%40–70%
Flow cap (stock)12–16 mm³/s10–14 mm³/s12–15 mm³/s
First layer15–20 mm/s, fan 0%15–20 mm/s, fan 0%15–20 mm/s, fan 0%

If PETG over-adheres to the bed, drop the bed by 5°C and use glue on textured PEI as a release layer. Find the temperature where stringing disappears, in 5°C steps, before you add speed.

Shared values for a sign face​

ItemValueWhere it applies
Layer height, visible face0.16–0.20 mmLetter front, diffuser frame
Layer height, structure0.24–0.28 mmBrackets, internal ribs
Top patternMonotonic linesWide caps, rear flanges
SeamAligned on the backNo random seam on the front
Wall orderOuter wall first, or a fixed outer-then-inner orderKeep the machine default if it is already the quality preset
Minimum layer time8–12 sStops small tips from melting
0.6 mm nozzleLayer 0.28–0.32 mm, outer wall 60–90 mm/sLarge internal structure. Keep 0.4 mm for fine strokes on the face

A 0.6 mm nozzle is for saving time. The wider line raises the required flow immediately, so apply 80% of the stock hotend flow table again. Splitting the face and the interior by nozzle produces fewer complaints than printing everything at 0.6 mm.

Order of application​

  1. Set nozzle temperature for that spool on a temperature tower, on a 5°C grid.
  2. Calibrate flow so the wall thickness matches.
  3. Reduce corner over-extrusion with a Pressure Advance or Linear Advance pattern.
  4. Print one letter coupon at the low end of the outer-wall speed in the table.
  5. Raise infill speed only after you inspect face layer lines, the seam, and joint holes.
  6. Save the passing profile as machine_material_nozzle_date, and use that profile's estimated time in the quote.

Do not raise production speed without a coupon. One failed print's material and bed time belongs in the failure-rate line of Pricing.